Case one: when a large area of the picture looks hazy, the membrane pressure is usually insufficient. Increase the pressure of the cold laminator and check that both ends of the roller are evenly adjusted.
Case two: small bubbles appear when the print surface carries dust or when the film is applied too quickly. Clean the print with a lint-free cloth and reduce the feeding speed.
Case three: curling at the roll edges points to uneven tension. Rewind the film and align the release paper before restarting.
Case four: a silvery sheen on dark areas means the adhesive has not fully wetted out. Allow the laminated print to rest for 24 hours at room temperature before judging the result.
Case five: visible texture on glossy prints usually means the wrong film side was used. The release paper with the printed grid must always face away from the print.
Store rolls horizontally in a dry room at 18-25 °C and keep them sealed until use. TOPLON technical support can help you tune your machine for a specific film series.